Texin® 260
热塑性聚氨酯弹性体(聚酯)
Texin 260 resin is an aromatic polyester-based thermoplastic polyurethane with a Shore hardness of approximately 60D. It can be processed by injection molding; extrusion processes are not recommended.
特性 | - 抗撞击性良好、良好的柔韧性、良好耐磨损性、耐燃油性、耐油性能、韧性良好
|
用途 | |
机构评级 | - FDA 21 CFR 177.1680、FDA 21 CFR 177.2600
|
外观 | |
加工方法 | |
密度 / 比重 |
|
|
|
-- | 1.22 |
| ASTM D792 |
-- | 1.22 | g/cm³ | ISO 1183 |
收缩率 |
|
|
|
流动 : 0.100 in | 8.0E-3 | in/in | ASTM D955 |
横向流动 : 0.100 in | 8.0E-3 | in/in | ASTM D955 |
横向流量 : 0.100 in | 0.80 | % | ISO 2577 |
流量 : 0.100 in | 0.80 | % | ISO 2577 |
肖氏硬度 (邵氏 D) | 60 |
| ASTM D2240, ISO 868 |
弯曲模量 |
|
|
|
73°F | 43000 | psi | ASTM D790 |
73°F | 42900 | psi | ISO 178 |
泰伯耐磨性 |
|
|
|
1000 Cycles, 1000 g, H-18 转轮 | 50.0 | mg | ASTM D1044 |
1000 Cycles, 1000 g, H-18 转轮 | 50.0 | mg | ISO 4649 |
拉伸应力 |
|
| ASTM D412, ISO 37 |
50%应变 | 2900 | psi |
|
100%应变 | 3210 | psi |
|
300%应变 | 5800 | psi |
|
抗张强度 (屈服) | 8700 | psi | ASTM D412, ISO 37 |
伸长率 (断裂) | 420 | % | ASTM D412, ISO 37 |
撕裂强度 |
|
|
|
-- 2 | 999 | lbf/in | ASTM D624 |
-- | 1000 | lbf/in | ISO 34-1 |
压缩永久变形 |
|
| ASTM D395B |
73°F, 22 hr | 27 | % |
|
73°F, 22 hr 3 | 21 | % |
|
158°F, 22 hr | 55 | % |
|
158°F, 22 hr 3 | 35 | % |
|
巴肖氏弹性 | 35 | % | ASTM D2632 |
如需科思创原厂物性表及相关文件,请联系我们工作人员,谢谢!