Stanyl® TQ261F2
聚酰胺 46
产品说明:
10% Glass Reinforced, Heat Stabilized
Special Features:
Stanyl® is our high-performance polyamide 46 used for applications in automotive, E&E, gears and outdoor power equipments.
Stanyl is a high performance polyamide that provides unmatched performance and value for demanding applications in which superior heat resistance, design stiffness, wear & friction and process flow qualities are required.
Because Stanyl retains its mechanical properties at high temperatures up to 220°C, this makes it ideal for extremely high-performance applications, where it outperforms PPA, PA6T, PA9T, and often PPS and LCP.
填料/增强材料 | |
添加剂 | |
特性 | |
加工方法 | |
树脂ID (ISO 1043) | |
密度 | 1.22 | g/cm³ | ISO 1183 |
吸水率 |
|
| ISO 62 |
饱和, 73°F | 11 | % |
|
平衡, 73°F, 50% RH | 3.1 | % |
|
拉伸模量 | 653000 | psi | ISO 527-2 |
拉伸应力 (断裂) | 16700 | psi | ISO 527-2 |
拉伸应变 (断裂) | 4.0 | % | ISO 527-2 |
弯曲模量 | 580000 | psi | ISO 178 |
简支梁缺口冲击强度 (73°F) | 3.8 | ft·lb/in² | ISO 179/1eA |
热变形温度 (264 psi, 未退火) | 536 | °F | ISO 75-2/A |
玻璃转化温度 2 | 167 | °F | ISO 11357-2 |
熔融温度 2 | 563 | °F | ISO 11357-3 |
干燥温度 | 176 | °F |
干燥时间 | 4.0 到 8.0 | hr |
料筒后部温度 | 536 到 608 | °F |
料筒中部温度 | 572 到 608 | °F |
料筒前部温度 | 572 到 608 | °F |
射嘴温度 | 572 到 608 | °F |
加工(熔体)温度 | 581 到 608 | °F |
模具温度 | 176 到 248 | °F |
注射速度 | 中等偏快 |
|
背压 | 290 到 1450 | psi |
螺杆压缩比 | 2.5:1.0 |
|
如需恩骅力(Envalior)原厂物性表及相关文件,请联系我司工作人员,谢谢!