Products

Texin® 1210

Texin® 1210

Manufacturer: Covestro
Produced At:
 Europe / China
Product Category: TPU
Product No: Texin 1210 
Product Quantity: 25KG / BAG
Product Features: 
Abrasion Resistant,Chemical Resistant,Food Contact Acceptable,Low Gel,Medium Clarity,Oil Resistant,Solvent Resistant

Texin® 1210

Thermoplastic Polyurethane Elastomer (Polyester)
Product Description:

Texin 1210 resin is an aromatic polyester-based thermoplastic polyurethane with a Shore hardness of approximately 92A.


Features 
  • Abrasion Resistant,Chemical Resistant,Food Contact Acceptable,Low Gel,

  • Medium Clarity,Oil Resistant,Solvent Resistant

Uses 
  • Cable Jacketing,Film,Footwear,Hose,Profiles,Sheet,Tubing
Agency Ratings 
  • FDA 21 CFR 177.1680,FDA 21 CFR 177.2600 
Appearance 
  • Natural Color

Processing Method 
  • Extrusion,Injection Molding 
Physical
Nominal Value
Unit
Test Method
Density / Specific Gravity



--
1.22

ASTM D792
--
1.22
g/cm³
ISO 1183
Hardness
Nominal Value
Unit
Test Method
Durometer Hardness (Shore A)
92

ASTM D2240, ISO 868
Mechanical
Nominal Value
Unit
Test Method
Flexural Modulus


ASTM D790, ISO 178
73°F
10600
psi

158°F
4600
psi

Taber Abrasion Resistance



1000 Cycles, 1000 g, H-18 Wheel
27.0
mg
ASTM D1044
1000 Cycles, 1000 g, H-18 Wheel
27.0
mg
ISO 4649
Elastomers
Nominal Value
Unit
Test Method
Tensile Stress


ASTM D412, ISO 37
100% Strain
1410
psi

300% Strain
2900
psi

Tensile Strength (Yield)
5800
psi
ASTM D412, ISO 37
Tensile Elongation (Break)
510
%
ASTM D412, ISO 37
Tear Strength



-- 2
737
lbf/in
ASTM D624
--
740
lbf/in
ISO 34-1
Compression Set 3


ASTM D395B, ISO 815
73°F, 22 hr
16
%

158°F, 22 hr
43
%

Thermal
Nominal Value
Unit
Test Method
Glass Transition Temperature
6.80
°F
DMA
Vicat Softening Temperature
190
°F
ISO 306/50, ASTM D1525 4
Injection
Nominal Value
Unit

Drying Temperature - Desiccant Dryer
178 to 219
°F

Drying Time - Desiccant Dryer
2.0
hr

Suggested Max Moisture
< 0.030
%

Suggested Max Regrind
20
%

Rear Temperature
360 to 385
°F

Middle Temperature
370 to 399
°F

Front Temperature
379 to 405
°F

Nozzle Temperature
385 to 410
°F

Processing (Melt) Temp
376 to 399
°F

Mold Temperature
61 to 100
°F

Injection Pressure
6000 to 15000
psi

Injection Rate
Moderate


Back Pressure
< 800
psi

Screw Speed
40 to 80
rpm

Cushion
< 0.125
in

Injection Notes
Hold Pressure: 60 to 80% of Injection Pressure
Extrusion
Nominal Value
Unit

Drying Temperature
178 to 219
°F

Drying Time
2.0
hr

Suggested Max Regrind
20
%

Cylinder Zone 1 Temp.
360 to 390
°F

Cylinder Zone 2 Temp.
360 to 399
°F

Cylinder Zone 3 Temp.
360 to 399
°F

Melt Temperature
376 to 399
°F

Die Temperature
370 to 399
°F



Products are widely used in plastic modification, automotive, construction, electrical and electronic, industrial, daily necessities and other fields