Desmopan® 5377A
Thermoplastic Polyurethane Elastomer (Ester/Ether)
Extrusion- and injection molding grade; improved microbial resistance; Improved hydrolysis resistance; Application; Cable sheathings; Textile coating; Wristwatch straps; hard to soft systems
RoHS Compliance | |
Processing Method | - Extrusion,Injection Molding
|
Density |
|
|
|
73°F | 1.14 | g/cm³ | ISO 1183 |
-- | 0.0412 | lb/in³ | ISO 1183 3 |
Shore Hardness |
|
|
|
Shore A, 1 sec, 73°F | 77 |
| ISO 7619 |
Shore D, 1 sec, 73°F | 28 |
| ISO 7619 |
Shore A, 3 sec | 77 |
| ISO 868 3 |
Shore D, 15 sec | 28 |
| ISO 868 3 |
Tensile Stress 4 |
|
| DIN 53504 |
Break, 73°F | 3920 | psi |
|
10% Strain, 73°F | 189 | psi |
|
50% Strain, 73°F | 522 | psi |
|
100% Strain, 73°F | 711 | psi |
|
300% Strain, 73°F | 1290 | psi |
|
Tensile Strain 4 (Break, 73°F) | 640 | % | DIN 53504 |
Abrasion Resistance 5 | 80.0 | mm³ | ISO 4649 |
Tensile Storage Modulus |
|
| ISO 6721 |
-4°F | 26107 | psi |
|
68°F | 4206 | psi |
|
140°F | 3046 | psi |
|
Tear Strength 6 (73°F) | 230 | lbf/in | ISO 34-1 |
Compression Set |
|
| ISO 815 |
73°F, 72 hr | 20 | % |
|
158°F, 24 hr 5 | 43 | % |
|
158°F, 24 hr 7 | 29 | % |
|
Rebound Resilience | 45 | % | ISO 4662 |
Drying Temperature | < 176 | °F |
|
Processing (Melt) Temp | 356 to 392 | °F |
|
Mold Temperature | 68 to 104 | °F |
|
Drying Temperature | < 176 | °F |
|
Melt Temperature | 338 to 374 | °F |
|